|本期目录/Table of Contents|

[1]崔子文,景元蓉,刘广永,等.增容剂对硅橡胶/热塑性聚氨酯热塑性硫化胶性能的影响[J].合成橡胶工业,2022,5:370-375.
 CUI Zi-wen,JING Yuan-rong,LIU Guang-yong,et al.Effect of compatibilizers on properties of silicone rubber/thermoplastic polyurethane thermoplastic vulcanizates[J].China synthetic rubber industy,2022,5:370-375.
点击复制

增容剂对硅橡胶/热塑性聚氨酯热塑性硫化胶性能的影响(PDF)

《合成橡胶工业》[ISSN:1000-1255/CN:62-1036/TQ]

期数:
2022年5期
页码:
370-375
栏目:
出版日期:
2022-09-15

文章信息/Info

Title:
Effect of compatibilizers on properties of silicone rubber/thermoplastic polyurethane thermoplastic vulcanizates
文章编号:
1000-1255(2022)05-0370-05
作者:
崔子文景元蓉刘广永杜爱华?鄢
青岛科技大学 橡塑材料与工程教育部重点实验室, 山东 青岛 266042
Author(s):
CUI Zi-wen JING Yuan-rong LIU Guang-yong DU Ai-hua
Key Laboratory of Rubber-Plastics of Ministry of Education, Qingdao University of Science and Technology, Qingdao 266042, China
关键词:
热塑性硫化胶动态硫化甲基乙烯基硅橡胶热塑性聚氨酯增容剂力学性能
Keywords:
thermoplastic vulcanizate dynamic vulcanization methyl vinyl silicone rubber thermoplastic polyurethane compatibilizer mechanical property
分类号:
TQ 333.93
DOI:
DOI:10.19908/j.cnki.ISSN1000-1255.2022.05.0370
文献标识码:
B
摘要:
采用动态硫化法制备了甲基乙烯基硅橡胶(MVQ)/热塑性聚氨酯(TPU)共混型热塑性硫化胶(TPV),考察了增容剂的种类及用量对TPV力学性能及加工流变性能的影响。结果表明,随着增容剂用量的增加,TPV的力学性能呈先上升后下降的趋势。相比于乙烯丙烯酸共聚物和乙烯与乙酸乙烯嵌段共聚物,用聚烯烃弹性体接枝马来酸酐(POE-g-MAH)作为增容剂时TPV的力学性能更为优异。3种增容剂均能提高TPV中MVQ相与TPU相的相容性。当POE-g-MAH的用量为6份时,TPV中MVQ相与TPU相的玻璃化转变温度靠近程度最大,两相界面较为模糊,增容效果最佳。
Abstract:
Methyl vinyl silicone rubber (MVQ)/thermoplastic polyurethane (TPU) blend thermoplastic vulcanizate (TPV) was prepared by dynamic vulcanization. The effects of type and amount of compatibilizers on mechanical properties and rheological properties of TPV were investigated. The results showed that the mechanical properties of TPV increased firstly and then decreased with the increase of compatibilizer amount. The mechanical properties of TPV were better when polyolefin elastomer grafted maleic anhydride (POE-g-MAH) was used as compatibilizer compared to ethylene acrylic copolymer and ethylene and vinyl acetate block copolymer. And all three kinds of compatibilizers could improve the compatibility of MVQ phase with TPU phase in TPV. When the amount of POE-g-MAH was 6 phr, the glass transition temperature of MVQ phase and TPU phase in TPV was the closest, the interface between the two phases was blurred and the capacitance effect was the best.

参考文献/References

[1] Ning Nanying, Li Shangqing, Wu Hanguang, et al. Preparation, microstructure, and microstructure-properties relationship of thermoplastic vulcanizates (TPVs): A review[J]. Progress in Polymer Science,2017,79:61-97.[2] Chatterjee T, Basu D, Das A, et al. Super thermoplastic vulcanizates based on carboxylated acrylonitrile butadiene rubber (XNBR) and polyamide (PA 12)[J]. European Polymer Journal,2016,78(5):235-252. [3] Ibrahim A, Dahlan M D. Thermoplastic natural rubber blends[J]. Progress in Polymer Science,1998,23(4):665-706.[4] Tang Yanchun, Lu Kai, Cao Xiaojun, et al. Nanostructured thermoplastic vulcanizates by selectively cross-linking a thermoplastic blend with similar chemical structures[J]. Industrial & Engineering Chemistry Research,2013,52(35):12613-12621.[5] Lu K, Duin M V, Loos J, et al. On the volume organisation of thermoplastic vulcanisates (TPVs) as revealed by scanning transmission electron microscopy (STEM) tomography [J]. Polymer,2012,53(19):4171-4177.[6] Ning Nanying, Hua Yueqing, Wu Hanguang, et al. Novel heat and oil-resistant thermoplastic vulcanizates based on ethylene-vinyl acetate rubber/poly(vinylidene fluoride)[J]. RSC Advances,2016,94(6):91594-91602. [7] Ning Nanying, Li Xiangyan, Tian Hongchi, et al. Unique microstructure of an oil resistant nitrile butadiene rubber/polypropylene dynamically vulcanized thermoplastic elastomer[J]. RSC Advances,2017,7(9):5451-5458.[8] Ma Piming, Xu Pengwu, Liu Wangcheng, et al. Bio-based poly(lactide)/ethylene-co-vinyl acetate thermoplastic vulcanizates by dynamic crosslinking: Structure vs property[J]. RSC Advances, 2015,5(21):15962-15968. [9] Chatterjee T. Novel thermoplastic vulcanizates (TPVs) based on silicone rubber and polyamide exploring peroxide cross-linking [J]. Express Polymer Letters,2014,8(4):220-231.[10] Ma Piming, Xu Pengwu, Zhai Yinghao, et al. Biobased poly(lactide)/ethylene-co-vinyl acetate thermoplastic vulcanizates: Morphology evolution, superior properties, and partial degradability[J]. ACS Sustainable Chemistry Engineering,2015,3(9):2211-2219.[11] Liu Hongzhi, Chen Feng, Liu Bo, et al. Super toughened poly(lactic acid) ternary blends by simultaneous dynamic vulcanization and interfacial compatibilization[J]. Macromolecules, 2010,43(14):6058-6066.[12] Ning Nanying, Hu Linjia, Yao Pengjun, et al. Study on the microstructure and properties of bromobutyl rubber (BIIR)/polyamide-12 (PA 12) thermoplastic vulcanizates (TPVs)[J]. Journal of Applied Polymer Science,2016, 133(8):e 43043.